STAINLESS STEELS
Material
Sintering
Cycle
r
g/cm3
E
GPa
Rm
MPa
Rr0.2
MPa
(static)
HRB
A5
%
AISI 304L
SL DA
SH DA
SH V
6.4
6.5
6.6
105
115
120
260
360
260
200
225
90
55
55
<0.5
5
12
AISI 316L
SL DA
SH DA
SH V
6.4
6.5
6.6
105
115
120
240
380
240
170
230
100
55
55
20
<0.5
5
12
AISI 410
SL DA + HT
6.5
125
>620
.
23
(HRC)
<0.5
AISI 430
SL V
SL V
6.4
6.6
.
350
430
180
260
82
91
.

Key:
SL DA - Sintered at 1150°C, (in dissociated ammonia: nitrogen pick up!)
SH DA - Same as SL DA, but sintered at 1290°C SL V - Sintered at 1150°C in pure hydrogen or vacuum
SH V - Same as SL V, but sintered at 1290°C
HT - Hardening and stress relieving

Data source: National and International Standards,
published in 'Guide to Design of Sintered Parts' and reprinted with permission of Assinter, Italy