FATIGUE STRENGTH OF SINTERED STEELS - AXIAL LOADING
Material
r
g/cm3
Prod
Cycle
Endurance Limits - N/mm2; Ps = 50%
Kt = 1
Kt = 2.8
R = 0
R = -1
R = 0
R = -1
SAE 1015
7.87
172
190
86
95
Nodular cast iron GH40-60
7.30
133
160
65
78
Fe-0.45P
6.8
7.1
SL
SL
77
108
91
126
45
55
56
68
Fe-1.5Cu
7.1
SL
81
100
48
58
Fe - 1.5Cu Carbonitrided
7.1
SL + CN
164
245
110
158
Fe - 1.5Cu - 0.6C
7.2
7.4
SL
PS+R+SL
130
145
165
172
64
80
84
100
Fe-1.5Cu-0.6C hardened and
tempered
7.1
SL+H1
155
222
70
102
Fe-2.0Cu-2.5Ni
7.1
SH1
119
145
64
79